Haynes International
Investor Relations
Customer Portal
English
日本語
中文
español
800.354.0806
765.456.6000
The Home of HASTELLOY® and HAYNES® Alloys
When autocomplete results are available use up and down arrows to review and enter to select.
Our Company
Company Overview
Locations and Directions
Investor Relations
Corporate Governance
Corporate Governance Guidelines
Corporate Policies
Human Trafficking Policy
Human Rights Policy
Conflicts Minerals Policy
Insider Trading Policy
Gift Policy
Cancellation Policy
Anti-Harassment Policy
Anti-Corruption Policy
Health, Safety, Environmental, and Quality Policy
Energy Policy
Code of Business Conduct and Ethics
Suppliers and Third Party Intermediaries
EthicsPoint Whistleblower Hotline
Conduct and Ethics Compliance
Directors and Executive Officers
Composition of Board Committees
Board Committee Charters
Sustainability
Environmental
Social
Governance
Our Positive Impact
Health, Safety, Environmental, and Quality
Health, Safety, Environmental, and Quality Policy
MSDS/Safety Data Sheets
Safety Data Sheets, English
Safety Data Sheets, Chinese
Safety Data Sheets, Czech
Safety Data Sheets, French
Safety Data Sheets, German
Safety Data Sheets, Italian
Safety Data Sheets, Japanese
Safety Data Sheets, Korean
Safety Data Sheets, Spanish
Energy Policy
Accreditations and Approvals
REACh
Trademarks
Our Heritage
Our Founder, Elwood Haynes
Our Company History
Our Milestones
Our Contributions to History
Careers
News
Markets
Aerospace
Power Generation
Chemical Processing
Emerging Technologies
Other Markets
Alloys
Alloy Portfolio
High-temperature Alloys
HAYNES® 25 alloy
HAYNES® 75 alloy
HAYNES® 188 alloy
HAYNES® 214® alloy
HAYNES® 230® alloy
HAYNES® 233™ alloy
HAYNES® 242® alloy
HAYNES® 244® alloy
HAYNES® 263 alloy
HAYNES® 282® alloy
HAYNES® 556® alloy
HAYNES® 617 alloy
HAYNES® 625 alloy
HAYNES® 625SQ® alloy
HAYNES® 718 alloy
HAYNES® HR-120® alloy
HAYNES® HR-160® alloy
HAYNES® HR-224® alloy
HAYNES® HR-235® alloy
MULTIMET® alloy
HAYNES® NS-163® alloy
HAYNES® R-41 alloy
HASTELLOY® S alloy
HASTELLOY® W alloy
HAYNES® Waspaloy alloy
HASTELLOY® X alloy
HAYNES® X-750 alloy
Corrosion-resistant Alloys
HASTELLOY® B-3® alloy
HASTELLOY® C-4 alloy
HASTELLOY® C-22® alloy
HASTELLOY® C-22HS® alloy
HASTELLOY® C-276 alloy
HASTELLOY® C-2000® alloy
HASTELLOY® G-30® alloy
HASTELLOY® G-35® alloy
HASTELLOY® HYBRID-BC1® alloy
HASTELLOY® N alloy
ULTIMET® alloy
Titanium Alloy
HAYNES® Ti-3Al-2.5V alloy
Alloy Nominal Compositions
Product Forms
Sheet and Plate
Wire and Welding
Pipe and Tubing
Bar and Billet
Fittings and Flanges
Welding and Fabrication
Welding and Fabrication Overview
Wire and Welding Product Forms
Hot-working
Cold-working
Welding and Joining
Heat Treatment
Machining
Grinding
Descaling and Pickling
Welding SmartGuide
Welding and Fabrication Brochure
Corrosion Guide
Introduction
Alloy Backgrounds
Alloy Groups
Metallurgy
Corrosive Environments
Wear Background
Abrasion
Erosion
Metal‐to‐Metal Sliding Wear
Corrosion Alloy Manual
Alloy Innovation
Alloy Development
Alloy Manufacturing
Alloy Technical Support
Specifications and Codes
Accreditations and Approvals
MSDS/Safety Data Sheets
Trademarks
Technical Library
Sales and Service
Sales and Service
Sales Office and Service Center Locations
Request for Quote
Terms and Conditions of Sale
Nickel Surcharges
Cancellation Policy
Export Compliance Policy Letter
Due Diligence
Incoterms®
Alloys and Products Brochure
Processing Capabilities
Bar Saw Cutting
Laser Cutting
Near-net Shaped Cut Parts
Plasma Cutting
Precision Shearing
Virtek® Laser QC®
Waterjet Cutting
Contact
Sales
Technical Support
Investor Relations
Careers
General Information
HASTELLOY® C-4 alloy
Home
Alloys
Alloy Portfolio
Corrosion-resistant Alloys
HASTELLOY® C-4 alloy
Tensile Strength and Elongation
HASTELLOY® C-4 alloy
Principal Features
Nominal Composition
Thermal Stability (T-T-S Chart)
Iso-Corrosion Diagrams
Comparative 0.1 mm/y Line Plots
Selected Corrosion Data
Resistance to Pitting and Crevice Corrosion
Resistance to Stress Corrosion Cracking
Physical Properties
Tensile Strength and Elongation
Hardness
Welding and Fabrication
Specifications and Codes
Disclaimer
Alloy Brochure
ASP.sfctrlpresentation_openaccessdataprovider_7b98424546ba62e18cdfff0000376e70_ascx
HASTELLOY® C-4 alloy
Principal Features
Nominal Composition
Thermal Stability (T-T-S Chart)
Iso-Corrosion Diagrams
Comparative 0.1 mm/y Line Plots
Selected Corrosion Data
Resistance to Pitting and Crevice Corrosion
Resistance to Stress Corrosion Cracking
Physical Properties
Tensile Strength and Elongation
Hardness
Welding and Fabrication
Specifications and Codes
Disclaimer
Alloy Brochure
Tensile Strength and Elongation
Form
Test Temperature
Thickness
0.2% Offset
Yield Strength
Ultimate Tensile
Strength
Elongation
°F
°C
in
mm
ksi
MPa
ksi
MPa
%
Sheet
RT
RT
0.065
1.7
60.3
416
111.4
768
52
Sheet
400
204
0.065
1.7
58.5
403
102.4
706
49
Sheet
600
316
0.065
1.7
53.8
371
97.9
675
52
Sheet
800
427
0.065
1.7
46.4
320
95.2
656
64
Sheet
RT
RT
0.125
3.2
61.0
421
116.2
801
54
Sheet
400
204
0.125
3.2
46.4
320
98.3
678
54
Sheet
600
316
0.125
3.2
43.9
303
97.5
672
59
Sheet
800
427
0.125
3.2
43.9
303
93.4
644
62
Sheet
1000
538
0.125
3.2
43.4
299
93.5
645
55
Sheet
RT
RT
0.156
4.0
53.0
365
113.5
783
55
Sheet
400
204
0.156
4.0
39.9
275
99.9
689
55
Sheet
600
316
0.156
4.0
36.1
249
95.3
657
61
Sheet
800
427
0.156
4.0
36.2
250
95.1
656
68
Plate
RT
RT
0.250
6.3
48.8
336
111.3
767
58
Plate
400
204
0.250
6.3
42.8
295
104.0
717
54
Plate
600
316
0.250
6.3
40.8
281
103.3
712
55
Plate
800
427
0.250
6.3
37.0
255
99.0
683
60
Plate
RT
RT
0.375
9.5
51.6
356
114.7
791
59
Plate
400
204
0.375
9.5
43.6
301
105.4
727
56
Plate
600
316
0.375
9.5
39.1
270
102.1
704
59
Plate
800
427
0.375
9.5
37.4
258
96.3
657
62
Plate
1000
538
0.375
9.5
33.0
228
93.3
643
52
Plate
RT
RT
0.500
12.7
48.6
335
116.8
805
63
Plate
400
204
0.500
12.7
38.3
264
105.2
725
61
Plate
600
316
0.500
12.7
35.8
247
102.5
707
65
Plate
800
427
0.500
12.7
34.2
236
99.8
688
66
Plate
1000
538
0.500
12.7
29.8
205
92.1
635
71