Samples mill annealed and cold worked yielded the following room temperature tensile results:

Cold Work Yield Strength Ultimate Tensile Strength Elongation
% ksi MPa ksi MPa %
0 74 510 134 924 57
10 112 772 150 1034 38
20 142 979 167 1151 26
30 168 1158 191 1317 14
40 194 1338 215 1482 8