Thickness Temperature 0.2% Offset Yield Strength Ultimate Tensile Strength Elongation
in/mm °F °C ksi MPa ksi MPa %
Sheet, Cold Rolled

&
Solution-Annealed

0.125/3.2 RT RT 58.7 405 122.0 841 61.6
200 93 52.2 360 117.6 811 66.1
300 149 48.3 333 114.4 789 64.5
400 204 45.0 310 110.6 763 63.3
500 260 42.4 292 109.4 754 67.9
600 316 41.1 283 108.0 745 68.5
700 371 40.0 276 108.3 747 76.9
800 427 40.6 280 112.8 778 75.3
Plate, Hot Rolled

&
Solution-Annealed

0.75/19.1 RT RT 52.5 362 117.4 809 70.5
200 93 47.4 327 112.9 778 74.8
300 149 42.7 294 108.7 749 74.8
400 204 38.8 268 104.8 723 74.6
500 260 35.7 246 102.4 706 74.7
600 316 35.6 245 100.4 692 71.1
700 371 34.8 240 99.8 688 74.0
800 427 32.7 225 99.0 683 76.3
Bar, Hot Rolled

&
Solution-Annealed

1.0/25.4 RT RT 55.9 385 120.6 832 63.0
200 93 50.4 347 115.8 798 73.6
300 149 45.1 311 111.5 769 72.8
400 204 41.9 289 107.8 743 72.1
500 260 39.6 273 105.2 725 72.7
600 316 37.1 256 103.5 714 72.0
700 371 36.6 252 103.3 712 72.0
800 427 37.2 256 102.3 705 74.1

RT= Room Temperature

Tensile Data for Weldments

• Transverse samples from welded plates of thickness 12.7 mm (0.5 in).
• Welding products made from same heat of HYBRID-BC1® alloy.

Welding Process Consumable Diameter Temperature 0.2% Offset
Yield Strength
Ultimate
Tensile Strength
Elongation
- in/mm °F °C ksi MPa ksi MPa %
Gas Tungsten Arc
GTAW (TIG)
0.125/3.2 RT RT 69.4 478 122.0 841 40.9
200 93 60.7 419 114.4 789 37.0
300 149 58.0 400 109.7 756 40.1
400 204 56.7 391 104.8 723 36.2
500 260 51.4 354 103.9 716 40.2
600 316 50.9 351 100.9 696 39.0
700 371 47.0 324 99.3 685 41.3
800 427 51.5 355 100.3 692 41.1
Synergic Gas

MetalArc
GMAW (MIG)

0.75/19.1 RT RT 72.6 501 121.1 835 37.2
200 93 66.4 458 115.3 795 39.7
300 149 63.5 438 109.7 756 37.6
400 204 58.3 402 104.3 719 39.3
500 260 59.2 408 98.8 681 33.7
600 316 59.9 413 102.8 709 42.5
700 371 58.7 405 99.7 687 37.2
800 427 60.3 416 99.2 684 38.8
Shielded Metal

Arc(SMAW)

1.0/25.4 RT RT 75.0 517 121.5 838 30.2
200 93 67.2 463 114.3 788 28.6
300 149 57.0 393 108.8 750 32.0
400 204 58.8 405 103.7 715 30.1
500 260 60.2 415 103.3 712 32.3
600 316 57.5 396 101.4 699 31.2
700 371 54.7 377 97.4 672 31.3
800 427 54.6 376 97.6 673 30.8

All Weld Tensile Metal Data

• Bar Samples of Diameter 12.7 mm (0.5 in) from GMAW (MIG) Cruciforms

Welding Process Consumable Diameter Temperature 0.2% Offset Yield Strength Ultimate Tensile Strength Elongation
- in/mm °F °C ksi MPa ksi MPa %
Synergic Gas

MetalArc
GMAW (MIG)

0.045/1.1 RT RT 73.8 509 110.8 764 47.7
200 93 68.9 475 104.8 723 46.1
300 149 64.8 447 101.6 701 50.8
400 204 62.3 430 96.8 667 47.2
500 260 62.6 432 93.8 647 46.0
600 316 61.2 422 94.4 651 51.3
700 371 59.8 412 91.6 632 49.5
800 427 58.8 405 88.9 613 50.9