Impact Strength

These impact strengths (averages from several tests) were generated using Charpy V-notch samples, machined from plates of thickness 10 mm and 25.4 mm.

Plate Thickness Test Temperature Impact Strength Number of Tests
in mm °F °C ft.lbf J
0.394 10 RT RT 340 461 6
0.394 10 -320 -196 418 567 6
1 25.4 RT RT 345 468 9
1 25.4 -320 -196 421 571 6