ULTIMET® alloy Site
Principal Features
Applications
Erosion
Galling
Abrasion Wear
Localized Corrosion
Aqueous Corrosion
Isocorrosion Curves
Physical Properties
Hardness
Tensile Data
High Temperature Corrosion
Welding
Health and Safety
Weld Overlay
Machining
Availability
ULTIMET® alloy
Technical Briefs
ULTIMET® alloy
Wire Information
Metallurgist Support
Sales Office Addresses
Tubular Products
Fittings & Flanges
|
| |
Typical Physical Properties |
| |
| Physical Properties |
Temp., °F |
British Units |
Temp., °C |
Metric Units |
|
| Density |
75 |
0.306 lb/in.3 |
24 |
8.47 g/cm.3 |
| Melting Temperature |
2430-2470 |
|
1332-1354 |
|
|
| Electrical Resistivity |
75 |
34.2 microhm-in. |
23 |
0.87 microhm-m |
| |
212 |
35.4 microhm-in. |
100 |
0.89 microhm-m |
| |
392 |
36.6 microhm-in. |
200 |
0.93 microhm-m |
| |
572 |
38.1 microhm-in. |
300 |
0.96 microhm-m |
| |
752 |
39.3 microhm-in. |
400 |
1.00 microhm-m |
| |
932 |
40.5 microhm-in. |
500 |
1.03 microhm-m |
| |
1112 |
41.3 microhm-in. |
600 |
1.05 microhm-m |
|
Mean Coefficient of
Thermal Expansion |
78-200 |
7.2 microinches/in.-°F |
26-93 |
13.0 x 10-6 m/m-K |
| |
78-400 |
7.5 microinches/in.-°F |
26-204 |
13.5 x 10-6 m/m-K |
| |
78-600 |
7.8 microinches/in.-°F |
26-316 |
14.0 x 10-6 m/m-K |
| |
78-800 |
8.0 microinches/in.-°F |
26-427 |
14.5 x 10-6 m/m-K |
| |
78-1000 |
8.2 microinches/in.-°F |
26-538 |
14.8 x 10-6 m/m-K |
| |
78-1200 |
8.4 microinches/in.-°F |
26-649 |
15.1 x 10-6 m/m-K |
| |
78-1400 |
8.8 microinches/in.-°F |
26-760 |
15.9 x 10-6 m/m-K |
| |
78-1600 |
9.1 microinches/in.-°F |
26-871 |
16.4 x 10-6 m/m-K |
| |
78-1800 |
9.4 microinches/in.-°F |
26-982 |
16.9 x 10-6 m/m-K |
|
| Thermal Diffusivity |
73 |
5 x 10-3 in.2/sec. |
23 |
3.3 x 10-6 m2/sec. |
| |
212 |
5 x 10-3 in.2/sec. |
100 |
3.5 x 10-6 m2/sec. |
| |
392 |
6 x 10-3 in.2/sec. |
200 |
3.8 x 10-6 m2/sec. |
| |
572 |
6 x 10-3 in.2/sec. |
300 |
4.2 x 10-6 m2/sec. |
| |
752 |
7 x 10-3 in.2/sec. |
400 |
4.5 x 10-6 m2/sec. |
| |
932 |
7 x 10-3 in.2/sec. |
500 |
4.7 x 10-6 m2/sec. |
| |
1112 |
7 x 10-3 in.2/sec. |
600 |
5.0 x 10-6 m2/sec. |
|
| Thermal Conductivity |
73 |
85 Btu-in./ft.2 hr.-°F |
23 |
12.3 W/m-K |
| |
212 |
96 Btu-in./ft.2 hr.-°F |
100 |
13.8 W/m-K |
| |
392 |
108 Btu-in./ft.2 hr.-°F |
200 |
15.6 W/m-K |
| |
572 |
121 Btu-in./ft.2 hr.-°F |
300 |
17.5 W/m-K |
| |
752 |
134 Btu-in./ft.2 hr.-°F |
400 |
19.4 W/m-K |
| |
932 |
149 Btu-in./ft.2 hr.-°F |
500 |
21.5 W/m-K |
| |
1112 |
166 Btu-in./ft.2 hr.-°F |
600 |
23.9 W/m-K |
|
| Specific Heat |
73 |
0.109 Btu/lb.-°F |
23 |
456 J/kg-K |
| |
212 |
0.112 Btu/lb.-°F |
100 |
470 J/kg-K |
| |
392 |
0.115 Btu/lb.-°F |
200 |
482 J/kg-K |
| |
572 |
0.121 Btu/lb.-°F |
300 |
504 J/kg-K |
| |
752 |
0.126 Btu/lb.-°F |
400 |
525 J/kg-K |
| |
932 |
0.130 Btu/lb.-°F |
500 |
545 J/kg-K |
| |
1112 |
0.137 Btu/lb.-°F |
600 |
573 J/kg-K |
|
| Typical Dynamic Modulus of Elasticity |
Form |
Condition |
Test Temperature
|
Average Dynamic
Modulus of Elasticity |
|
°F |
°C |
106 psi |
GPa |
|
|
| Plate |
Heat-treated at 2050°F
Water Quenched |
400 |
204 |
31.2 |
215 |
|
600 |
316 |
29.9 |
206 |
800 |
427 |
28.6 |
197 |
1000 |
538 |
27.4 |
189 |
1200 |
649 |
26.1 |
180 |
|
|
|