Galling Test |
Galling Test (2722 kg/6000 lb. Load)
Room Temperature |
|
|
10 strokes/120° arc |
*GTA 2-layer deposit |
|
|
| |
| |
|
Degree of Damage, microns Load |
|
| Pin |
Block |
1361 kg
(3000 lb) |
2722 kg
(6000 lb) |
4082 kg
(9000 lb) |
|
|
|
| ULTIMET® alloy |
ULTIMET alloy |
2.9 |
2.7 |
2.0 |
|
| ULTIMET® alloy |
1045 Carbon Steel (HRC 32) |
7.4 |
6.6 |
8.2 |
|
| ULTIMET® alloy |
4140 Alloy Steel (HRC 46) |
2.3 |
2.7 |
2.5 |
|
| ULTIMET® alloy |
H-13 Tool Steel (HRC 48) |
2.1 |
2.1 |
2.0 |
|
| ULTIMET® alloy |
Type 304 Stainless Steel |
2.5 |
5.5 |
18.3 |
|
| ULTIMET® alloy |
Type 316L Stainless Steel |
1.4 |
1.2 |
0.7 |
|
| Type 316L Stainless Steel |
Type 316L Stainless Steel |
>100.0 |
- |
- |
|
| ULTIMET® alloy |
Type 410 Stainless Steel |
9.4 |
9.4 |
17.7 |
|
| ULTIMET® alloy |
17-4-PH® Stainless Steel (HRC 39) |
3.5 |
3.5 |
5.7 |
|
| 17-4-PH Stainless (HRC 39) |
17-4-PH® Stainless (HRC 39) |
57.8 |
>100.0 |
>100.0 |
|
| ULTIMET® alloy |
HASTELLOY® C-276 alloy |
11.4 |
14.6 |
17.6 |
|
| ULTIMET® alloy |
HAYNES® 718 alloy (HRC 47) |
7.1 |
8.5 |
11.7 |
|
| HAYNES® 718 alloy (HRC 47) |
HAYNES® 718 alloy (HRC 47) |
18.1 |
24.0 |
16.7 |
|
| ULTIMET® alloy |
STELLITE® 6** |
0.1 |
0.1 |
0.1 |
|
| ULTIMET® alloy |
STELLITE® 6H** |
0.1 |
0.1 |
0.1 |
|
| HAYNES® 6B alloy |
HAYNES® 6B alloy |
0.6 |
0.7 |
0.5 |
|
| NITRONIC® 60 alloy |
NITRONIC 60 alloy |
2.5 |
120.0 |
111.3 |
|
| |
|
|
|
|
|
All Wrought Products except:
** All-Weld-Metal, GTA weld type. |
| |