HAYNES® HR-160® alloy Site
Principal Features
Applications
High Temperature Resistance
Oxidation Resistance
Chloridation Resistance
Carburization Resistance
Nitriding Resistance
Waste Incineration Environments
Tensile Properties
Creep and Stress-Rupture
Physical Properties
Physical Metallurgy
Thermal Stability
Corrosion Resistance
Welding
Machining
Health and Safety Information
HAYNES® HR-160® alloy
Technical Briefs
HAYNES® HR-160 ® alloy
Wire Information
Metallurgist Support
Sales Office Addresses
Tubular Products
Fittings & Flanges
|
| |
Typical Physical Properties |
| |
|
Temp., °F |
British Units |
Temp., °C |
Metric Units |
|
| Density |
Room |
0.292 lb/in. 3 |
Room |
8.08 g/cm. 3 |
| Melting Temperature |
2360-2500 |
|
1293-1370 |
|
|
| Electrical Resistivity |
Room |
43.8 microhm-in. |
Room |
111.2 microhm-cm |
|
200 |
44.3 microhm-in. |
100 |
112.8 microhm-cm |
|
400 |
45.2 microhm-in. |
200 |
114.7 microhm-cm |
|
600 |
46.1 microhm-in. |
300 |
116.7 microhm-cm |
|
800 |
46.9 microhm-in. |
400 |
118.6 microhm-cm |
|
1000 |
47.8 microhm-in. |
500 |
120.6 microhm-cm |
|
1200 |
48.3 microhm-in. |
600 |
122.4 microhm-cm |
|
1400 |
48.6 microhm-in. |
700 |
123.1 microhm-cm |
|
1600 |
48.9 microhm-in. |
800 |
123.8 microhm-cm |
|
1800 |
49.3 microhm-in. |
900 |
124.5 microhm-cm |
|
2000 |
49.6 microhm-in. |
1000 |
125.2 microhm-cm |
|
2200 |
49.9 microhm-in. |
1100 |
125.9 microhm-cm |
|
- |
- |
1200 |
126.7 microhm-cm |
|
| Thermal Diffusivity |
Room |
4.6 x 10-3 in.2 /sec. |
Room |
29.4 x 10 -3 cm2 /sec. |
|
212 |
4.8 x 10-3 in.2/sec. |
100 |
30.8 x 10 -3 cm2 /sec. |
|
392 |
5.2 x 10-3 in.2/sec. |
200 |
33.6 x 10 -3 cm2 /sec. |
|
572 |
5.7 x 10-3 in.2/sec. |
300 |
37.0 x 10 -3 cm2 /sec. |
|
752 |
6.3 x 10-3 in.2/sec. |
400 |
40.6 x 10 -3 cm2 /sec. |
|
932 |
6.9 x 10-3 in.2/sec. |
500 |
44.3 x 10 -3 cm2 /sec. |
|
1112 |
7.1 x 10-3 in.2/sec. |
600 |
45.6 x 10 -3 cm2 /sec. |
|
1292 |
7.3 x 10-3 in.2/sec. |
700 |
47.2 x 10 -3 cm2 /sec. |
|
1472 |
7.5 x 10-3 in.2/sec. |
800 |
48.6 x 10 -3 cm2 /sec. |
|
1652 |
7.5 x 10-3 in.2/sec. |
900 |
48.7 x 10 -3 cm2 /sec. |
|
1832 |
7.9 x 10-3 in.2/sec. |
1000 |
50.9 x 10 -3 cm2 /sec. |
|
2012 |
8.4 x 10-3 in.2/sec. |
1100 |
54.1 x 10 -3 cm2 /sec. |
|
2192 |
8.7 x 10-3 in.2/sec. |
1200 |
56.1 x 10 -3 cm2 /sec. |
|
| Thermal Conductivity |
Room |
75 Btu-in./ft.2 hr.-°F |
Room |
10.9 W/m-K |
|
200 |
82 Btu-in./ft.2 hr.-°F |
100 |
12.0 W/m-K |
|
400 |
95 Btu-in./ft.2 hr.-°F |
200 |
13.6 W/m-K |
|
600 |
108 Btu-in./ft.2 hr.-°F |
300 |
15.4 W/m-K |
|
800 |
126 Btu-in./ft.2 hr.-°F |
400 |
17.6 W/m-K |
|
1000 |
144 Btu-in./ft.2 hr.-°F |
500 |
19.9 W/m-K |
|
1200 |
162 Btu-in./ft.2 hr.-°F |
600 |
21.8 W/m-K |
|
1400 |
178 Btu-in./ft.2 hr.-°F |
700 |
24.7 W/m-K |
|
1600 |
185 Btu-in./ft.2 hr.-°F |
800 |
26.1 W/m-K |
|
1800 |
196 Btu-in./ft.2 hr.-°F |
900 |
26.9 W/m-K |
|
2000 |
213 Btu-in./ft.2 hr.-°F |
1000 |
28.7 W/m-K |
|
2200 |
228 Btu-in./ft.2 hr.-°F |
1100 |
31.1 W/m-K |
|
- |
- |
1200 |
32.9 W/m-K |
|
|
|
Temp., °F |
British Units |
Temp., °C |
Metric Units |
|
|
| Specific Heat |
Room |
0.110 Btu/lb.-°F |
Room |
462 J/Kg-K |
|
200 |
0.116 Btu/lb.-°F |
100 |
487 J/Kg-K |
|
400 |
0.121 Btu/lb.-°F |
200 |
506 J/Kg-K |
|
600 |
0.125 Btu/lb.-°F |
300 |
521 J/Kg-K |
|
800 |
0.131 Btu/lb.-°F |
400 |
542 J/Kg-K |
|
1000 |
0.136 Btu/lb.-°F |
500 |
562 J/Kg-K |
|
1200 |
0.151 Btu/lb.-°F |
600 |
597 J/Kg-K |
|
1400 |
0.159 Btu/lb.-°F |
700 |
653 J/Kg-K |
|
1600 |
0.164 Btu/lb.-°F |
800 |
672 J/Kg-K |
|
1800 |
0.167 Btu/lb.-°F |
900 |
689 J/Kg-K |
|
2000 |
0.171 Btu/lb.-°F |
1000 |
704 J/Kg-K |
|
2200 |
0.175 Btu/lb.-°F |
1100 |
719 J/Kg-K |
|
- |
- |
1200 |
732 J/Kg-K |
|
Dynamic Modulus of
|
Room |
30.6 x 106 psi |
Room |
211 GPa |
| Elasticity |
100 |
30.5 x 106 psi |
40 |
210 GPa |
|
200 |
30.1 x 106 psi |
90 |
208 GPa |
|
300 |
29.6 x 106 psi |
150 |
204 GPa |
|
400 |
29.1 x 106 psi |
205 |
201 GPa |
|
500 |
28.6 x 106 psi |
260 |
197 GPa |
|
600 |
27.8 x 106 psi |
315 |
192 GPa |
|
700 |
27.1 x 106 psi |
370 |
187 GPa |
|
800 |
26.5 x 106 psi |
425 |
183 GPa |
|
900 |
26.1 x 106 psi |
480 |
180 GPa |
|
1000 |
25.6 x 106 psi |
540 |
177 GPa |
|
1100 |
25.1 x 106 psi |
595 |
173 GPa |
|
1200 |
24.4 x 106 psi |
650 |
168 GPa |
|
1300 |
23.7 x 106 psi |
705 |
163 GPa |
|
1400 |
22.9 x 106 psi |
760 |
158 GPa |
|
1500 |
22.4 x 106 psi |
815 |
154 GPa |
|
1600 |
21.7 x 106 psi |
870 |
150 GPa |
|
1700 |
21.1 x 106 psi |
925 |
145 GPa |
|
1800 |
19.8 x 106 psi |
980 |
137 GPa |
|
| Mean Coefficient of |
78-200 |
7.2 microinches/in.-°F |
25-95 |
13.0 106m/m-ºC |
| Thermal Expansion |
78-400 |
7.6 microinches/in.-°F |
25-205 |
13.7 106m/m-ºC |
|
78-600 |
7.9 microinches/in.-°F |
25-315 |
14.0 106m/m-ºC |
|
78-800 |
8.1 microinches/in.-°F |
25-425 |
14.4 106m/m-ºC |
|
78-1000 |
8.3 microinches/in.-°F |
25-540 |
14.9 106m/m-ºC |
|
78-1200 |
8.6 microinches/in.-°F |
25-600 |
15.5 106m/m-ºC |
|
78-1400 |
8.9 microinches/in.-°F |
25-700 |
15.7 106m/m-ºC |
|
78-1600 |
9.2 microinches/in.-°F |
25-800 |
16.6 106m/m-ºC |
|
78-1800 |
9.5 microinches/in.-°F |
25-900 |
17.1 106m/m-ºC |
|
|
| |
|
|
|