skip to:
page content
|
links on this page
|
site navigation
|
footer (site information)
Haynes International, Inc. 800-354-0806 765-456-6012
Home
Corrosion-Resistant Alloys
High-Temperature Alloys
Welding Information
Fabrication
Specifications
CRA Fabrication Brochure
|
Corrosion Resistant Alloys
|
HTA Fabrication Brochure
|
High-Temperature Alloys
|
Welding Information
|
CRA Specifications
|
HTA Specifications
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
subglobal7 link
|
subglobal7 link
|
subglobal7 link
|
subglobal7 link
|
subglobal7 link
|
subglobal7 link
|
subglobal7 link
subglobal8 link
|
subglobal8 link
|
subglobal8 link
|
subglobal8 link
|
subglobal8 link
|
subglobal8 link
|
subglobal8 link
HAYNES
®
718 alloy Information
An aged-hardenable Ni-Fe-Cr-Cb-Mo-Ti-Al alloy that combines excellent strength to 1200°F (650°C) with good ductility, formability, and weldability.
HAYNES
®
718 alloy Site
Principal Features
Creep and Stress-Rupture Strengths
Tensile Properties
Modulus of Elasticity
Physical Properties
Fabrication and Welding
Health and Safety
HAYNES
®
718 alloy
Technical Briefs
HAYNES
®
718 alloy
Wire Information
Metallurgist Support
Sales Office Addresses
Tubular Products
Fittings & Flanges
Tensile Data
Cold-Rolled, Solution-Treated and Aged* (Sheet)
Test
Temperature
Ultimate
Tensile Strength
Yield Strength
at 0.2% Offset
Elongation in
2 in. (50.8 mm)
°F
°C
Ksi
MPa
Ksi
MPa
%
Room
Room
202.3
1395
170.4
1175
22.3
1000
540
164.1
1130
144.0
995
24.4
1200
650
167.6
1155
144.8
1000
19.9
1400
760
124.1
855
108.6
750
10.2
1600
870
43.9
305
30.6
420
27.7
1800
980
20.9
145
13.0
90
37.0
2000
1095
11.2
77
5.8
40
38.5
*Limited data