HAYNES® 718 alloy Site
Principal Features
Creep and Stress-Rupture Strengths
Tensile Properties
Modulus of Elasticity
Physical Properties
Fabrication and Welding
Health and Safety
HAYNES® 718 alloy
Technical Briefs
HAYNES® 718 alloy
Wire Information
Metallurgist Support
Sales Office Addresses
Tubular Products
Fittings & Flanges
|
| |
Typical Physical Properties |
| |
| |
Temp., °F |
British Units |
Temp., °C |
Metric Units |
| Density |
Room |
0.297 lb/in.3 |
Room |
8.23 g/cm.3 |
| Melting Range |
2300-2435 |
|
1260-1335 |
|
|
| Electrical Resistivity |
Room |
47.5 microhm-in. |
Room |
121 microhm-cm |
| |
200 |
48.0 microhm-in. |
100 |
122 microhm-cm |
| |
400 |
49.4 microhm-in. |
200 |
125 microhm-cm |
| |
600 |
50.3 microhm-in. |
300 |
127 microhm-cm |
| |
800 |
50.7 microhm-in. |
400 |
129 microhm-cm |
| |
1000 |
51.6 microhm-in. |
500 |
130 microhm-cm |
| |
1200 |
52.0 microhm-in. |
600 |
132 microhm-cm |
| |
1400 |
52.2 microhm-in. |
700 |
132 microhm-cm |
| |
1600 |
52.1 microhm-in. |
800 |
132 microhm-cm |
| |
1800 |
52.4 microhm-in. |
900 |
133 microhm-cm |
| |
|
|
1000 |
133 microhm-cm |
|
Mean Coefficient of
Thermal Expansion |
70-200 |
7.1 microinches/in.-°F |
25-100 |
12.8 μm/m-°C |
| |
70-400 |
7.5 microinches/in.-°F |
25-200 |
13.5 μm/m-°C |
| |
70-600 |
7.7 microinches/in.-°F |
25-300 |
13.8 μm/m-°C |
| |
70-800 |
7.9 microinches/in.-°F |
25-400 |
14.1 μm/m-°C |
| |
70-1000 |
8.0 microinches/in.-°F |
25-500 |
14.3 μm/m-°C |
| |
70-1200 |
8.4 microinches/in.-°F |
25-600 |
14.8 μm/m-°C |
| |
70-1400 |
8.9 microinches/in.-°F |
25-700 |
15.5 μm/m-°C |
| |
70-1600 |
9.4 microinches/in.-°F |
25-800 |
16.3 μm/m-°C |
| |
|
|
25-900 |
17.2 μm/m-°C |
|
| Thermal Conductivity |
Room |
79 Btu-in./ft.2 hr.-°F |
Room |
11.4 W/m-K |
| |
200 |
87 Btu-in./ft.2 hr.-°F |
100 |
12.6 W/m-K |
| |
400 |
100 Btu-in./ft.2 hr.-°F |
200 |
14.3 W/m-K |
| |
600 |
112 Btu-in./ft.2 hr.-°F |
300 |
15.9 W/m-K |
| |
800 |
124 Btu-in./ft.2 hr.-°F |
400 |
17.5 W/m-K |
| |
1000 |
136 Btu-in./ft.2 hr.-°F |
500 |
19.0 W/m-K |
| |
1200 |
148 Btu-in./ft.2 hr.-°F |
600 |
20.6 W/m-K |
| |
1400 |
161 Btu-in./ft.2 hr.-°F |
700 |
22.2 W/m-K |
| |
1600 |
173 Btu-in./ft.2 hr.-°F |
800 |
23.8 W/m-K |
| |
1800 |
186 Btu-in./ft.2 hr.-°F |
900 |
25.4 W/m-K |
| |
- |
- |
1000 |
27.1 W/m-K |
|
|
|
|