| Temperature, °F |
British Units |
Temperature, °C |
Metric Units |
|
Room |
29.0 x 106 psi |
Room |
200 GPa |
200 |
28.4 x 106 psi |
100 |
195 GPa |
400 |
27.6 x 106 psi |
200 |
191 GPa |
600 |
26.7 x 106 psi |
300 |
185 GPa |
800 |
25.8 x 106 psi |
400 |
179 GPa |
1000 |
24.8 x 106 psi |
500 |
173 GPa |
1200 |
23.7 x 106 psi |
600 |
167 GPa |
1400 |
22.3 x 106 psi |
700 |
159 GPa |
1600 |
20.2 x 106 psi |
800 |
149 GPa |
1800 |
17.4 x 106 psi |
900 |
134 GPa |
- |
- |
1000 |
117 GPa |
|
|