Fittings & Flanges
|
| |
Typical Physical Properties |
| |
| |
Temp., °F |
British Units |
Temp., °C |
Metric Units |
| Density |
Room |
0.305 lb/in.3 |
Room |
8.44 g/cm.3 |
| Melting Temperature |
2350-2460 |
|
1290-1350 |
|
|
| Electrical Resistivity |
Room |
50.8 microhm-in. |
Room |
129 microhm-cm |
| |
200 |
52.0 microhm-in. |
100 |
132 microhm-cm |
| |
400 |
52.8 microhm-in. |
200 |
134 microhm-cm |
| |
600 |
53.1 microhm-in. |
300 |
135 microhm-cm |
| |
800 |
53.5 microhm-in. |
400 |
136 microhm-cm |
| |
1000 |
54.3 microhm-in. |
500 |
137 microhm-cm |
| |
1200 |
54.3 microhm-in. |
600 |
138 microhm-cm |
| |
1400 |
53.9 microhm-in. |
700 |
138 microhm-cm |
| |
1600 |
53.5 microhm-in. |
800 |
137 microhm-cm |
| |
1800 |
53.1 microhm-in. |
900 |
136 microhm-cm |
| |
|
|
1000 |
135 microhm-cm |
|
Mean Coefficient of
Thermal Expansion |
70-200 |
7.1 microinches/in.-°F |
25-100 |
12.8 10-6 μ/m-°C |
| |
70-400 |
7.3 microinches/in.-°F |
25-200 |
13.1 10-6 μ/m-°C |
| |
70-600 |
7.5 microinches/in.-°F |
25-300 |
13.4 10-6 μ/m-°C |
| |
70-800 |
7.7 microinches/in.-°F |
25-400 |
13.8 10-6 μ/m-°C |
| |
70-1000 |
8.0 microinches/in.-°F |
25-500 |
14.2 10-6 μ/m-°C |
| |
70-1200 |
8.4 microinches/in.-°F |
25-600 |
14.8 10-6 μ/m-°C |
| |
70-1400 |
8.7 microinches/in.-°F |
25-700 |
15.4 10-6 μ/m-°C |
| |
70-1600 |
9.2 microinches/in.-°F |
25-800 |
16.0 10-6 μ/m-°C |
| |
70-1800 |
9.6 microinches/in.-°F |
25-900 |
16.7 10-6 μ/m-°C |
| |
|
|
25-1000 |
17.4 10-6 μ/m-°C |
|
| Thermal Conductivity |
Room |
68 Btu-in./ft.2 hr.-°F |
Room |
9.8 W/m-K |
| |
200 |
75 Btu-in./ft.2 hr.-°F |
100 |
10.9 W/m-K |
| |
400 |
87 Btu-in./ft.2 hr.-°F |
200 |
12.5 W/m-K |
| |
600 |
98 Btu-in./ft.2 hr.-°F |
300 |
13.9 W/m-K |
| |
800 |
109 Btu-in./ft.2 hr.-°F |
400 |
15.3 W/m-K |
| |
1000 |
121 Btu-in./ft.2 hr.-°F |
500 |
16.9 W/m-K |
| |
1200 |
132 Btu-in./ft.2 hr.-°F |
600 |
18.3 W/m-K |
| |
1400 |
144 Btu-in./ft.2 hr.-°F |
700 |
19.8 W/m-K |
| |
1600 |
158 Btu-in./ft.2 hr.-°F |
800 |
21.5 W/m-K |
| |
1800 |
175 Btu-in./ft.2 hr.-°F |
900 |
23.4 W/m-K |
| |
|
|
1000 |
25.6 W/m-K |
|
| Specific Heat |
Room |
0.098 Btu/lb.-°F |
Room |
410 J/kg-K |
| |
200 |
0.102 Btu/lb.-°F |
100 |
428 J/kg-K |
| |
400 |
0.109 Btu/lb.-°F |
200 |
455 J/kg-K |
| |
600 |
0.115 Btu/lb.-°F |
300 |
477 J/kg-K |
| |
800 |
0.122 Btu/lb.-°F |
400 |
503 J/kg-K |
| |
1000 |
0.128 Btu/lb.-°F |
500 |
527 J/kg-K |
| |
1200 |
0.135 Btu/lb.-°F |
600 |
552 J/kg-K |
| |
1400 |
0.141 Btu/lb.-°F |
700 |
576 J/kg-K |
| |
1600 |
0.148 Btu/lb.-°F |
800 |
600 J/kg-K |
| |
1800 |
0.154 Btu/lb.-°F |
900 |
625 J/kg-K |
| |
|
|
1000 |
648 J/kg-K |
|
|
|
|
|