skip to:
page content
|
links on this page
|
site navigation
|
footer (site information)
Haynes International, Inc. 800-354-0806 765-456-6012
Home
Corrosion-Resistant Alloys
High-Temperature Alloys
Welding Information
Fabrication
Specifications
CRA Fabrication Brochure
|
Corrosion Resistant Alloys
|
HTA Fabrication Brochure
|
High-Temperature Alloys
|
Welding Information
|
North American Service Centers
|
International Service Centers
|
subglobal5 link
|
subglobal5 link
|
subglobal5 link
|
subglobal5 link
|
subglobal5 link
subglobal6 link
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
|
subglobal6 link
subglobal7 link
|
subglobal7 link
|
subglobal7 link
|
subglobal7 link
|
subglobal7 link
|
subglobal7 link
|
subglobal7 link
subglobal8 link
|
subglobal8 link
|
subglobal8 link
|
subglobal8 link
|
subglobal8 link
|
subglobal8 link
|
subglobal8 link
HAYNES
®
214
®
alloy Information
A nickel-chromium-aluminum-iron alloy with outstanding resistance to oxidation.
HAYNES
®
214
®
alloy Site
Principal Features
Typical Applications
Oxidation Resistance
Carburization Resistance
Resistance to Chlorine-Bearing
Environments
Nitriding Resistance
Physical Properties
Modulus of Elasticity
Tensile Properties
Creep and Rupture Properties
Thermal Stability
Fabrication Characteristics
Welding
Health and Safety
HAYNES
®
214
®
alloy
Technical Briefs
HAYNES
®
214
®
alloy
Wire Information
Metallurgist Support
Sales Office Addresses
Tubular Products
Fittings & Flanges
Dynamic Modulus of Elasticity
Temp., °F
Dynamic
Modulus of
Elasticity,
10
6
psi
Temp., °C
Dynamic
Modulus of
Elasticity,
GPa
Room
31.6 x 10
6
psi
Room
218 GPa
200
30.6 x 10
6
psi
100
210 GPa
400
29.6 x 10
6
psi
200
204 GPa
600
28.7 x 10
6
psi
300
199 GPa
800
27.4 x 10
6
psi
400
190 GPa
1000
25.3 x 10
6
psi
500
184 GPa
1200
23.9 x 10
6
psi
600
177 GPa
1400
22.3 x 10
6
psi
700
170 GPa
1600
20.2 x 10
6
psi
800
162 GPa
1800
19.0 x 10
6
psi
900
151 GPa
-
-
1000
137 GPa