HASTELLOY® G-35® alloy Site
Principal Features
Chemical Composition
Physical Properties
Corrosion Data
Iso-Corrosion Diagrams
Mechanical Properties
Welding and Fabrication
Machining
Specifications
HASTELLOY® G-35 alloy
Technical Briefs
HASTELLOY® G-35 alloy
Wire Information
Metallurgist Support
Sales Office Addresses
Tubular Products
Fittings & Flanges
|
| |
Physical Properties |
| |
Physical Property
|
Metric Units |
British Units |
|
Density |
RT |
8.22 g/cm.3 |
RT |
0.297 lb/in.3 |
|
Electrical Resistivity
|
RT |
1.18 μohm.m |
RT |
46.5 μohm.in |
100°C |
1.19 μohm.m |
212°F |
46.9 μohm.in |
|
200°C |
1.20 μohm.m |
392°F |
47.2 μohm.in |
|
300°C |
1.21 μohm.m |
572°F |
47.6 μohm.in |
|
400°C |
1.22 μohm.m |
752°F |
48.0 μohm.in |
|
500°C |
1.24 μohm.m |
932°F |
48.8 μohm.in |
|
600°C |
1.25 μohm.m |
1112°F |
49.2 μohm.in |
|
Thermal Conductivity
|
RT |
10 W/m.°C |
RT |
70 btu.in/h.ft2.°F |
100°C |
12 W/m.°C |
212°F |
85 btu.in/h.ft2.°F |
|
200°C |
14 W/m.°C |
392°F |
95 btu.in/h.ft2.°F |
|
300°C |
16 W/m.°C |
572°F |
110 btu.in/h.ft2.°F |
|
400°C |
18 W/m.°C |
752°F |
125 btu.in/h.ft2.°F |
|
500°C |
19 W/m.°C |
932°F |
135 btu.in/h.ft2.°F |
|
600°C |
23 W/m.°C |
1112°F |
160 btu.in/h.ft2.°F |
|
Mean Coefficient of Thermal Expansion |
21-100°C |
12.3 μm/m.°C |
70-212°F |
6.8 μin/in.°F |
21-200°C |
12.6 μm/m.°C |
70-392°F |
7.0 μin/in.°F |
21-300°C |
13.2 μm/m.°C |
70-572°F |
7.3 μin/in.°F |
|
21-400°C |
13.4 μm/m.°C |
70-752°F |
7.5 μin/in.°F |
|
21-500°C |
13.6 μm/m.°C |
70-932°F |
7.6 μin/in.°F |
|
21-600°C |
14.1 μm/m.°C |
70-1112°F |
7.8 μin/in.°F |
|
Thermal Diffusivity
|
RT |
0.028 cm²/s |
RT |
0.11 ft²/h |
100°C |
0.031 cm²/s |
212°F |
0.12 ft²/h |
|
200°C |
0.034 cm²/s |
392°F |
0.13 ft²/h |
|
300°C |
0.038 cm²/s |
572°F |
0.15 ft²/h |
|
400°C |
0.042 cm²/s |
752°F |
0.16 ft²/h |
|
500°C |
0.045 cm²/s |
932°F |
0.17 ft²/h |
|
600°C |
0.048 cm²/s |
1112°F |
0.19 ft²/h |
|
Specific Heat |
RT |
450 J/kg.°C |
RT |
0.11 btu/lb.°F |
|
100°C |
470 J/kg.°C |
212°F |
0.11 btu/lb.°F |
|
200°C |
490 J/kg.°C |
392°F |
0.12 btu/lb.°F |
|
300°C |
510 J/kg.°C |
572°F |
0.12 btu/lb.°F |
|
400°C |
530 J/kg.°C |
752°F |
0.13 btu/lb.°F |
|
500°C |
530 J/kg.°C |
932°F |
0.13 btu/lb.°F |
|
600°C |
600 J/kg.°C |
112°F |
0.14 btu/lb.°F |
|
Dynamic Modulus of Elasticity
(Young's Modulus) |
RT |
204 GPa |
RT |
29.6 x 106 psi |
316°C |
189 GPa |
600°F |
27.4 x 106 psi |
427°C |
183 GPa |
800°F |
26.5 x 106 psi |
538°C |
177 GPa |
1000°F |
25.7 x 106 psi |
649°C |
170 GPa |
1200°F |
24.7 x 106 psi |
|
Melting Range |
1332 - 1361°C |