Average Physical Properties |
| |
| Physical Property |
Temp., °F |
British Units |
Temp., °C |
Metric Units |
|
| Density |
72 |
0.321 lb/in.3 |
22 |
8.89 g/cm.3 |
| Melting Range |
2415-2500 |
|
1323-1371 |
|
|
| Electrical Resistivity |
75 |
51 microhm-in. |
24 |
1.30 microhm-m |
|
Mean Coefficient of
Thermal Expansion |
75-200 |
6.2 microinches/in.-°F |
24-93 |
11.2 x 10-6 m/m•K |
75-400 |
6.7 microinches/in.-°F |
24-204 |
12.0 x 10-6 m/m•K |
75-600 |
7.1 microinches/in.-°F |
24-316 |
12.8 x 10-6 m/m•K |
| |
75-800 |
7.3 microinches/in.-°F |
24-427 |
13.2 x 10-6 m/m•K |
| |
75-1000 |
7.4 microinches/in.-°F |
24-538 |
13.4 x 10-6 m/m•K |
|
| Thermal Conductivity |
-270 |
50 Btu-in./ft.2 hr.-°F |
-168 |
7.2 W/m•K |
| |
-100 |
60 Btu-in./ft.2 hr.-°F |
-73 |
8.6 W/m•K |
| |
0 |
65 Btu-in./ft.2 hr.-°F |
-18 |
9.4 W/m•K |
| |
100 |
71 Btu-in./ft.2 hr.-°F |
38 |
10.2 W/m•K |
| |
200 |
77 Btu-in./ft.2 hr.-°F |
93 |
11.1 W/m•K |
| |
400 |
90 Btu-in./ft.2 hr.-°F |
204 |
13.0 W/m•K |
| |
600 |
104 Btu-in./ft.2 hr.-°F |
316 |
15.0 W/m•K |
| |
800 |
117 Btu-in./ft.2 hr.-°F |
427 |
16.9 W/m•K |
| |
1000 |
132 Btu-in./ft.2 hr.-°F |
538 |
19.0 W/m•K |
|
Specific Heat
(Calculated) |
Room |
0.102 Btu/lb.-°F |
Room |
427 J/kg•K |
|
|
|