HASTELLOY® C-22® alloy Site
Principal Features
Laboratory Corrosion Tests
Field Evaluation
Typical Applications
Aqueous Corrosion Data
Resistance to Localized Attack
Thermal Stability
Isocorrosion Curves
Physical Properties
Hardness and Impact Strength
Tensile Data
Fabrication
Welding
Machining
HASTELLOY® C-22® alloy
Technical Briefs
HASTELLOY® C-22® alloy Wire Information
Metallurgist Support
Sales Office Addresses
Tubular Products
Fittings & Flanges
|
| |
Field Evaluations |
| |
Exhibits Excellent Corrosion Protection
Chemical Processing Industry |
Flue Gas Desulfurization (FGD) |
Reactor Vessel
10-15% Sulfuric Acid + Solids/Impurities
212°F (100°C) — 12 Months
|
Pulverized Coal Fire Unit
4.8% Sulfur Outlet Duct
129°F (54°C) — 27 Months
|
Corrosion Rate (mpy) |
Remarks |
|
Depth of Attack |
Pitting (in.) |
Crevice (in.) |
316L Stainless Steel |
>61 |
Sample Dissolved |
316L Stainless Steel |
0.011 |
0.015 |
Carpenter 20Cb-3® alloy |
>57 |
Sample Dissolved |
Alloy 904L |
0.010 |
0.005 |
| Alloy 825 |
>58 |
Sample Dissolved |
Jessop JS700 alloy |
0.010 |
0.011 |
HASTELLOY® B-2 alloy |
>58 |
Sample Dissolved |
HAYNES 625 alloy |
No Attack |
0.005 |
HAYNES® 625 alloy |
29 |
Severe Corrosion Attack |
HASTELLOY C-276 alloy |
No Attack |
0.007 |
HASTELLOY C-276 alloy |
28 |
Severe Corrosion Attack |
HASTELLOY C-22 alloy |
No Attack |
0.002 |
HASTELLOY C-22® alloy |
4.7 |
Slight Corrosion Attack |
|
|
|
Refinery Industry |
Chemical Waste Invineration |
Coke Refinery
Vaporizer
203°F (95°C) — 2 Months
|
Rotary Kiln Industiral Organic
Quench Duct
300°F (149°C) — 4 Months
|
Corrosion Rate (mpy) |
Remarks |
Corrosion Rate (mpy) |
Remarks |
316L Stainless Steel |
139 |
Severe Crevice Attack |
Carbon Steel |
>353 |
Severe Crevice Attack |
Carpenter 20Cb-3® alloy |
227 |
Partially Dissolved |
316L Stainless Steel |
>160 |
Partially Dissolved |
Avesta 254 SMO® alloy |
83 |
Pitting, Crevice Attack |
Avesta 254 SMO alloy |
83 |
Pitting, Crevice Attack |
Allegheny AL-6XN® alloy |
60 |
Pitting, Crevice Attack |
HAYNES 625 alloy |
64 |
Pitting, Crevice Attack |
HAYNES 625 alloy |
29 |
Pitting, Crevice Attack |
HASTELLOY C-276 alloy |
53 |
Pitting, Crevice Attack |
HASTELLOY C-22 alloy |
3.4 |
Slight Crevice Attack |
HASTELLOY C-22 alloy |
27 |
Slight Crevice Attack |
Pulp and Paper Industry |
Chemical Waste Incineration |
Ammonium Sulfite-Type Mill
C-Stage Washer
75°F (24°C) — 8 Months
|
Ammonia Stripping Process
Waste Water
160°F (71°C) — 3 Months
|
|
Depth of Attack |
|
Depth of Attack |
Pitting (in.) |
Crevice (in.) |
Pitting (in.) |
Crevice (in.) |
316L Stainless Steel |
0.030 |
0.045 |
Carbon Steel |
0.040 |
0.050 |
Alloy 904L |
0.023 |
0.029 |
316L Stainless Steel |
0.005 |
0.005 |
Avesta 254 SMO alloy |
0.015 |
No Attack |
Allegheny AL-6XN alloy |
0.005 |
No Attack |
HAYNES 625 alloy |
0.005 |
No Attack |
HAYNES 625 alloy |
0.004 |
No Attack |
HASTELLOY C-22 alloy |
0.002 |
No Attack |
HASTELLOY C-276 alloy |
No Attack |
No Attack |
|
|
|