Physical Properties |
| |
| Physical Property |
Metric Units |
British Units |
| Density |
RT |
8.50 g/cm. 3 |
RT |
0.307 lb/in. 3 |
| Electrical Resistivity |
RT |
1.28 µohm.m |
RT |
50.6 µohm.in |
|
100°C |
1.29 µohm.m |
200°F |
50.8 µohm.in |
|
200°C |
1.30 µohm.m |
400°F |
51.2 µohm.in |
|
300°C |
1.31 µohm.m |
600°F |
51.6 µohm.in |
|
400°C |
1.32 µohm.m |
800°F |
52.2 µohm.in |
|
500°C |
1.34 µohm.m |
1000°F |
52.9 µohm.in |
|
600°C |
1.35 µohm.m |
1200°F |
53.0 µohm.in |
| Thermal Conductivity |
RT |
9.1 W/m.°C |
RT |
63 btu.in/h.ft².°F |
|
100°C |
10.8 W/m.°C |
200°F |
74 btu.in/h.ft².°F |
|
200°C |
12.6 W/m.°C |
400°F |
88 btu.in/h.ft².°F |
|
300°C |
14.1 W/m.°C |
600°F |
99 btu.in/h.ft².°F |
|
400°C |
16.1 W/m.°C |
800°F |
114 btu.in/h.ft².°F |
|
500°C |
18.0 W/m.°C |
1000°F |
133 btu.in/h.ft².°F |
|
600°C |
21.6 W/m.°C |
1200°F |
162 btu.in/h.ft².°F |
| Mean Coefficient of Thermal Expansion |
25-100°C |
12.4 µm/m.°C |
77-200°F |
6.9 µin/in.°F |
| 25-200°C |
12.4 µm/m.°C |
77-400°F |
6.9 µin/in.°F |
|
25-300°C |
12.6 µm/m.°C |
77-600°F |
7.0 µin/in.°F |
|
25-400°C |
12.9 µm/m.°C |
77-800°F |
7.2 µin/in.°F |
|
25-500°C |
13.2 µm/m.°C |
77-1000°F |
7.4 µin/in.°F |
|
25-600°C |
13.3 µm/m.°C |
77-1200°F |
7.6 µin/in.°F |
| Thermal Diffusivity |
RT |
0.025 cm²/s |
RT |
0.10 ft²/h |
|
100°C |
0.029 cm²/s |
212°F |
0.11 ft²/h |
|
200°C |
0.033 cm²/s |
392°F |
0.13 ft²/h |
|
300°C |
0.036 cm²/s |
572°F |
0.14 ft²/h |
|
400°C |
0.040 cm²/s |
752°F |
0.16 ft²/h |
|
500°C |
0.043 cm²/s |
932°F |
0.17 ft²/h |
|
600°C |
0.047 cm²/s |
1112°F |
0.18 ft²/h |
| Specific Heat |
RT |
428 J/kg.°C |
RT |
0.10 btu/lb.°F |
|
100°C |
434 J/kg.°C |
212°F |
0.10 btu/lb.°F |
|
200°C |
443 J/kg.°C |
392°F |
0.11 btu/lb.°F |
|
300°C |
455 J/kg.°C |
572°F |
0.11 btu/lb.°F |
|
400°C |
468 J/kg.°C |
752°F |
0.11 btu/lb.°F |
|
500°C |
486 J/kg.°C |
932°F |
0.12 btu/lb.°F |
|
600°C |
536 J/kg.°C |
1112°F |
0.13 btu/lb.°F |
| Dynamic Modulus of Elasticity |
RT |
207 GPa |
RT |
30.0 x 10 6 psi |
| 316°C |
190 GPa |
600°F |
27.5 x 10 6 psi |
|
427°C |
177 GPa |
800°F |
25.6 x 10 6 psi |
|
538°C |
171 GPa |
1000°F |
24.8 x 10 6 psi |
|
649°C |
162 GPa |
1200°F |
23.5 x 10 6 psi |
| Melting Range |
1328-1358°C |
2422-2476°F |
|
|
|